= 0.1%
SRA = 0.3%
SRA = 0.5%
500
450
400
350
300
250
200
150
7
28
Curing times (days)
FIG. 1 - Values obtained with mortar containing CEM I 52.5 R cement, normalised sand and water, according
to the composition indicated in the EN 196-1 Standards
Contrasted-expansion air curing (+20°C and 50% R.H.) according to UNI 8147
450
Shrinkage/expansion (µm/m)
RA
S
re
u
c
pe
a
M
Without SRA
SRA = 0.1%
SRA = 0.3%
SRA = 0.5%
400
350
300
250
200
150
100
50
0
-50
1
28
-100
-150
-200
-250
Curing time (days)
FIG. 2 - Values obtained with mortar containing CEM I 52.5 R cement, normalised sand and water, according
to the composition indicated in the EN 196-1 Standards, and 7% of Expancrete admixture
Compressive strength (N/mm²)
Development of mechanical strength
60
55
50
45
40
35
30
Without SRA
SRA = 0.1%
SRA = 0.3%
SRA = 0.5%
25
20
15
10
5
0
0
7
14
21
28
Curing time (days)
FIG. 3 - Values obtained with mortar containing CEM I 52.5 R cement, normalised sand ... ascunde
Pentru noi, confidențialitatea dvs. este importantă
Portalul spatiulconstruit.ro folosește cookies pentru a asigura funcționalitatea și securitatea site-ului, pentru a personaliza conținutul și modul de interacțiune, pentru a oferi facilități de social media
și pentru a analiza modul în care este utilizat site-ul. Aceste cookies sunt stocate și prelucrate, de către noi sau partenerii noștri în conformitate cu toate reglementările în vigoare și toate standardele
de confidențialitate și securitate actuale.
Vă rugăm să rețineți că este posibil ca anumite prelucrări ale datelor dumneavoastră cu caracter personal să nu necesite consimțământul dumneavoastră, dar vă puteți exprima acordul cu privire la prelucrarea
realizată de către noi și partenerii noștri conform descrierii de mai sus utilizând butonul SUNT DE ACORD de mai jos.
Navigând în continuare, vă exprimați acordul implicit asupra folosirii cookie-urilor.